Copper Matt and White Crackle Raku Glaze Recipes

Copper Matt Raku, cone 010—06
Glaze Material
Percentage
Bone Ash 33%
Gerstley Borate 67
100%
Add: Copper Carbonate 8%
Cobalt Carbonate 2%
White Crackle Raku, cone 010—06
Glaze Material Percentage
Barium Carbonate 15%
Gerstley Borate 40
Nepheline Syenite 35
silica 10
100%

The copper matt glaze produces a range of colors, including lusters and opalescence, and is very receptive to post-fire reduction. Apply a thin coat of glaze then wipe off with a dry towel to achieve a matt, speckled surface. Use in combination with the white crackle glaze for a mottled effect.