All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
cedar-heights-gold-art 35.00
lizella 33.00
OM 4 Ball Clay 2.00
Fine Grog 20.00
ultra-fine-grog 10.00
Add Amount
darvan-(in-drops) 10.00
flax-fiber-(in-pinches) 1.00
paper-pulp-(in-percentage) 5.00
water-(in-percentage) 60.00

Instructions

Versatile, adhesive slip. Sticks to anything other than glossy surfaces. Relatively quick drying, low shrinkage. Good for attaching bone dry to bone dry clay, bisqueware to greenware, etc. Should be applied thick for best adhesion. To alter the recipe for a robust paper clay sculpture body, remove UF Grog and Darvan, change OM 4 to 10%, and add 2% bentonite.

 

This recipe was shared by Gabriel John Poucher in the May 2025 issue of Ceramics Monthly.