All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 16.00
Lithium 10.00
Whiting 8.00
Ferro Frit 3110 9.00
EPK Kaolin 15.00
Minspar 200 30.00
Silica 12.00
Add Amount
BENTONITE 2.00

Instructions

Apply this glaze thick with a large sumi or hake brush. I will also often utilize a syringe when trying to pool the glaze in certain areas or get into small spaces. This glaze runs significantly if layered thick and fired past cone 1. When firing, put a layer of a silica sand and alumina hydrate mixture on shelves to help work move and catch any glaze drips. 

  • For Brown/Gold: 
    • Add: Red Iron Oxide 15 %
  • For Gray/Green–Yellow/Green: 
    • Add: Nickel 1–5 %
  • For Mint Green: 
    • Add: Copper 1 %
    • Chrome 0.5 %
  • For Brown Green: 
    • Add: Chrome 0.5 %
  • For Mauve-Black: 
    • Add: Manganese 1–8 %

 

This recipe was shared by Anna Kruse in the June/July/August 2025 issue of Ceramics Monthly.