All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Soda Ash 10.00
Nepheline Syenite 10.00
Petalite 10.00
Grolleg 35.00
Helmar Kaolin 35.00

Instructions

This flashing slip recipe was given to me from Stephen Mickey. It’s a very nice slip in the wood or soda kiln with a nice range of color depending on your clay body. Apply thin to medium. I mix it to the consistency of whole milk.

This recipe was shared by Donovan Palmquist in the March 2025 issue of Ceramics Monthly.