How to Make a Carved Bisque Mold for Repeatable Raised Relief Designs
This handy trick will help you make consistent designs on your pots!
David Scott Smith
Carved decoration is lovely on ceramic pieces, but it also can be labor intensive. But in today's post we have a great way to create a repeatable design by creating a carved bisque mold.
In this post, an excerpt from the Pottery Making Illustrated archive, David Scott Smith shares how he throws, trims, and carves a bisque mold for a bowl. Brilliant! - Jennifer Poellot Harnetty, editor
PS. Check out the July/August 2020 issue of Pottery Making Illustratedto learn how David adds a foot and puts the finishing touches on his bowls!
Several years ago, I discovered an exciting way to create bowls with raised relief designs by using bisque-fired bowl molds on the pottery wheel.
Creating the Carved Bisque Mold
Begin by throwing a bowl on the wheel. Since it will be trimmed into a dome and carved, I usually prefer to use smooth clay with little or no grog. The walls of the bowl should be fairly thick—I want my mold to be durable for use after it has been
bisque fired.
Consider the pitch when making the bowl. If the sides of the bowl are steep and the carved design is deep or elaborate, I often have problems releasing the bowl from the mold. When clay is pressed against the bisque mold, it immediately begins to shrink
and constrict, which could make it difficult to remove from the mold, so I recommend starting with a fairly shallow bowl design.
After the bowl has been thrown on the wheel, attach a handle or knob inside the bowl on the bottom to help in releasing finished forms later on. Until the bowl is leather hard, leave it on the bat or wheel head, being careful not to distort the bowl or
rim. It’s very important that the bowl is perfectly round and symmetrical, so that after the bisque firing it sits flat and can be centered on the wheel head. When the bowl has dried to a leather-hard state, flip the bowl over and trim it into
a dome (1), then smooth with a damp sponge.
Carving Surface Decoration
I love carving leather-hard clay that’s slightly softer than a chocolate bar. My tools of choice: an X-Acto blade (preferably new), a needle tool with a bent tip (use a blowtorch to heat the end of the tool before bending), and a variety of mini-ribbon tools (2). I also prefer to work on a banding wheel.
I often sketch my design lightly with the needle tool (3). The bent tip allows me to drag the needle without creating burrs or scratching the surface too deeply. The mini ribbon tools are great for carving designs (4), but surface textures can also be created by pressing the ends of modeling tools or other objects into the surface (5). I use my X-Acto blade to carve designs, although to remove clay I must make two cuts from opposing angles (6) and take care not to create undercuts. For each cut made with the X-Acto blade, the blade is held flat at approximately a 45° angle from the surface.
Sometimes I like to carve deep marks when the bowl is a softer leather hard, and then make more marks later after the bowl has hardened. I think a variety of textures and carved lines can add interest and dimension to the finished design.
When the bowl is dry, take some time to clean up any burrs or undercuts before bisque firing the mold. A stiff bristle brush helps soften any unattractive or harsh features. I bisque fire the bowl mold only to cone 06–08
so that the clay remains porous and will absorb moisture from the pressed clay slab. Next, center the mold on a bat on the wheel head upside down with the carved dome facing up. Tip: I’m terribly inept at centering pots,
so I often cheat by first drawing concentric circles on my bat while it’s spinning, and use these lines to help me position my mold.
Roll out a soft slab to ¼–½ inch thick (depending on how heavy you want the bowl to be), smoothing out any blemishes or canvas texture with a damp sponge or rubber rib, and very carefully place it on the mold (7). Be careful
not to move the mold while placing the slab. A flat slab doesn’t like to bend over a bowl, and this next step takes some practice (just accept that the first few attempts may look weird). Press the clay onto the mold, starting at
the center and working down to the wheel head. Work in a spiral motion, moving the wheel head (by hand, don’t turn the wheel on) until the slab is firmly fastened to the mold, and the excess of the slab is pressed firmly to the bat.
Make sure there are several inches of slab stuck to the bat; this will secure the mold to the wheel head when the wheel is finally turned on. Pressing the slab onto the mold correctly is important. Use fingertips to work the clay into
the detail of the mold (8), while being careful to not move the slab once it has already been pressed into the texture. Any movement of the slab will create a tracer image (similar to a repeated pattern) effect. As I mentioned above, it
takes some practice, so don’t be discouraged if your first few tries are less than satisfactory. Turn on the wheel to slow to medium speed, and use a sponge to compress the slab against the mold. Next, trim away some of the excess
slab (9), leaving at least 2–3 inches. Make sure there is enough slab to cling to the plastic bat, so it doesn’t fly off the wheel.
Search the Daily
Published Mar 22, 2023
Carved decoration is lovely on ceramic pieces, but it also can be labor intensive. But in today's post we have a great way to create a repeatable design by creating a carved bisque mold.
In this post, an excerpt from the Pottery Making Illustrated archive, David Scott Smith shares how he throws, trims, and carves a bisque mold for a bowl. Brilliant! - Jennifer Poellot Harnetty, editor
PS. Check out the July/August 2020 issue of Pottery Making Illustrated to learn how David adds a foot and puts the finishing touches on his bowls!
Several years ago, I discovered an exciting way to create bowls with raised relief designs by using bisque-fired bowl molds on the pottery wheel.
Creating the Carved Bisque Mold
Begin by throwing a bowl on the wheel. Since it will be trimmed into a dome and carved, I usually prefer to use smooth clay with little or no grog. The walls of the bowl should be fairly thick—I want my mold to be durable for use after it has been bisque fired.
Consider the pitch when making the bowl. If the sides of the bowl are steep and the carved design is deep or elaborate, I often have problems releasing the bowl from the mold. When clay is pressed against the bisque mold, it immediately begins to shrink and constrict, which could make it difficult to remove from the mold, so I recommend starting with a fairly shallow bowl design.
After the bowl has been thrown on the wheel, attach a handle or knob inside the bowl on the bottom to help in releasing finished forms later on. Until the bowl is leather hard, leave it on the bat or wheel head, being careful not to distort the bowl or rim. It’s very important that the bowl is perfectly round and symmetrical, so that after the bisque firing it sits flat and can be centered on the wheel head. When the bowl has dried to a leather-hard state, flip the bowl over and trim it into a dome (1), then smooth with a damp sponge.
Carving Surface Decoration
I love carving leather-hard clay that’s slightly softer than a chocolate bar. My tools of choice: an X-Acto blade (preferably new), a needle tool with a bent tip (use a blowtorch to heat the end of the tool before bending), and a variety of mini-ribbon tools (2). I also prefer to work on a banding wheel.
I often sketch my design lightly with the needle tool (3). The bent tip allows me to drag the needle without creating burrs or scratching the surface too deeply. The mini ribbon tools are great for carving designs (4), but surface textures can also be created by pressing the ends of modeling tools or other objects into the surface (5). I use my X-Acto blade to carve designs, although to remove clay I must make two cuts from opposing angles (6) and take care not to create undercuts. For each cut made with the X-Acto blade, the blade is held flat at approximately a 45° angle from the surface.
Sometimes I like to carve deep marks when the bowl is a softer leather hard, and then make more marks later after the bowl has hardened. I think a variety of textures and carved lines can add interest and dimension to the finished design.
When the bowl is dry, take some time to clean up any burrs or undercuts before bisque firing the mold. A stiff bristle brush helps soften any unattractive or harsh features. I bisque fire the bowl mold only to cone 06–08 so that the clay remains porous and will absorb moisture from the pressed clay slab. Next, center the mold on a bat on the wheel head upside down with the carved dome facing up. Tip: I’m terribly inept at centering pots, so I often cheat by first drawing concentric circles on my bat while it’s spinning, and use these lines to help me position my mold.
Roll out a soft slab to ¼–½ inch thick (depending on how heavy you want the bowl to be), smoothing out any blemishes or canvas texture with a damp sponge or rubber rib, and very carefully place it on the mold (7). Be careful not to move the mold while placing the slab. A flat slab doesn’t like to bend over a bowl, and this next step takes some practice (just accept that the first few attempts may look weird). Press the clay onto the mold, starting at the center and working down to the wheel head. Work in a spiral motion, moving the wheel head (by hand, don’t turn the wheel on) until the slab is firmly fastened to the mold, and the excess of the slab is pressed firmly to the bat. Make sure there are several inches of slab stuck to the bat; this will secure the mold to the wheel head when the wheel is finally turned on. Pressing the slab onto the mold correctly is important. Use fingertips to work the clay into the detail of the mold (8), while being careful to not move the slab once it has already been pressed into the texture. Any movement of the slab will create a tracer image (similar to a repeated pattern) effect. As I mentioned above, it takes some practice, so don’t be discouraged if your first few tries are less than satisfactory. Turn on the wheel to slow to medium speed, and use a sponge to compress the slab against the mold. Next, trim away some of the excess slab (9), leaving at least 2–3 inches. Make sure there is enough slab to cling to the plastic bat, so it doesn’t fly off the wheel.
Unfamiliar with any terms in this article? Browse our glossary of pottery terms!
Related Content
Ceramic Artists
Functional Pottery
Ceramic Sculpture
Glaze Chemistry
High-Fire Glaze Recipes
Mid-Range Glaze Recipes
Low-Fire Glaze Recipes
Ceramic Colorants
Ceramic Glazes and Underglazes
Ceramic Raw Materials
Pottery Clay
Ceramic Decorating Tools
Ceramic Kilns
Making Clay Tools
Wheel Throwing Tools
Electric Kiln Firing
Gas Kiln Firing
Raku Firing
Salt Firing and Soda Firing
Wood Kiln Firing
Ceramic Decorating Techniques
Ceramic Glazing Techniques
Handbuilding Techniques
Making Ceramic Molds
Making Ceramic Tile
Wheel Throwing Techniques