Cracks tell a story, and if you pay attention to what they are saying, you can troubleshoot your drying and firing problems. While cracks can occur in clay bodies and in glazes, let’s first take a look at clay-body cracks.
Defining the Terms
Bone Dry: Clay that is dry to the touch but still has minimal amounts of mechanical and chemical water. It has no plasticity and is at its weakest point.
Clay Body: A combination of clay(s), fluxes, and fillers to achieve a specific firing range, forming method, fired color, and kiln atmosphere.
Clay Platelets: Microscopic, flat, hexagonal clay plates that, when combined with water, achieve plasticity. The ratio of the long dimension to the plate thickness is approximately 10 to 1. Clay platelets can range in size from 100 microns to 0.1 micron average particle dilatometer.1 (1 micron = 1 millionth of a meter).
Dry Strength: The capacity of clay in the dry state to resist cracking, breaking, or deformation when subjected to stress.
Leather Hard: Clay that is firm but pliable and has enough moisture to be manipulated in a forming process and has not reached the brittle stage in drying. It can be trimmed and supports its own shape.
Quartz Inversion: A reversible transition occurring in the crystalline structure of quartz at approximately 1063°F (533°C), resulting in a sudden change in volume and expansion/contraction.
Tensile Stress: The internal resisting force in a cross section of a material when subjected to pulling forces. Clay is weak in tensile loads and strong in compressive loads.
Thermal Expansion: Increase in the size of ceramic material caused by an increase in temperature.
What Exactly Is a Crack?
A crack occurs when a clay body splits apart internally, indicating a stress overload exceeding its strength, such as uneven shrinkage in drying or firing, high tensile loads, and rapid heating or cooling. This dynamic mechanism (movement of clay particles in response to a force acting on it) also applies to cracks in glazes.
As pottery was produced on a larger commercial scale, a method of crack identification was required. This system offered a standardized pathway to solving cracks.2
When observing a crack, it might be useful to ask the following:
Where is the crack?
When did it form?
What does it look like?
What stress produced the crack?
At what stage did the crack start?
Round-Edge and Sharp-Edge Cracks (1, 2)
The first step in solving a crack defect is to determine if it’s a sharp-edge crack (imagine you hit the fired pot with a hammer) or a round-edge crack (fired glaze rolls back from the edge of the crack). The correct diagnosis at this point is critical.
Round-edge cracks start either in the clay-body formula, forming, drying, or bisque firing stages, and then the glaze was applied over the existing crack. Some round-edge cracks are difficult to observe in leather-hard, bone-dry, or bisque stages. However, when in doubt, run a slightly damp sponge over the suspect areas. Moisture will collect in the crack, making it visible. These cracks will have a round edge as opposed to a sharp hairline fault when fired.
Factors Producing Round-Edge Cracks
Incorrect Clay Body: Often the incorrect clay body is the first suspect in producing a crack. Some clay-body formulas are more likely to crack than others, caused by either end of their plasticity spectrum. Specifically, short clay bodies (low plasticity) can break or tear when subjected to forming stresses, resulting in cracking upon drying. An extremely plastic clay body can have high percentages of fine-grained clays such as ball clays or bentonite. These clays have a high water state for plasticity, causing excessive shrinkage and cracking upon drying. Conversely, clay bodies with small, medium, and largeplatelet sizes can increase packing within the structure, which reduces shrinking and drying cracks. An important first step in preventing potential cracks is to choose the appropriate clay body for the forming method.
Shrinkage (3): Different rates of shrinkage in drying or bisque firing can cause stress cracks in several ways. The use of two or more different clay bodies can induce cracking in drying or bisque firing due to different shrinkage rates exceeding the clays’ ability to withstand tensile stress. During a firing, each clay can have different rates of thermal expansion in heating and cooling, leading to a failure.
When a dry piece of clay is attached to another piece, and as the two exhibit different shrinkage rates in drying or bisque firing, a crack, or a semi-dry clay face with small movable unstable particles interrupts the joined surface, it acts as a parting layer between the two assembled sections.3
Cracks can result when thin sections are joined to thicker sections of clay. Thin sections of clay dry quickly and begin to shrink, while thicker sections of clay containing water have not begun to shrink at an equivalent rate.
Bone-Dry Clay Breakage (4): Bone-dry pots, brittle and lacking moisture, are at their weakest state. The clay platelets are tightly packed but with little or no free water film to bind them weakly together. The pot may not appear to be cracked, but cracks can develop in the later stages of forming or drying. At the point of impact, compressive stress is generated while producing tensile stress on the opposite side of the impact. Tensile stress is greater than the clay’s ability to withstand the impact, forming micro-cracks which can propagate.4
Trimming Crack (5): The tip of the trim tool applies compressive pressure as it comes in contact with the clay’s surface, causing shear and tensile stresses. The bone-dry or semi-moist clay plus the pressure from the trimming tool are enough to stress the clay and exceed its dry strength. This type of crack happens around the outer or inner circumference of a pot’s foot and can spread as the pot dries, further extending from the original weak point. The less water contained in the pot, the more likely this type of crack will develop.5
S-Type Cracks (6): This frequent type of crack in wheel-thrown pottery is noticed upon the clay’s drying. Centered clay should be thoroughly compressed on the bottom of the form before pulling up the walls. A more effective approach is, after centering the clay, to pull it up into a cylinder shape, then compress it onto the bat. This aligns the clay platelets and prevents S-type cracks. Shallow elongated S-type cracks can sometimes occur in slab-built or wheel-thrown forms due to not wedging the clay before forming.
O- and C-Type Cracks (7): As the name implies, cracks are circular and frequently appear in the drying stage. They are caused by excess water or slurry (a clay/water mixture) being left in the ware. Cracks are frequently seen in the outer rims of thrown plates where the slurry mixture has been thrown by the centrifugal force of the wheel. Often the slurry is difficult to distinguish from the surrounding clay. The same process occurs at the bottom inner edge of a thrown cylinder where the slurry has not been removed. O-type cracks occur when the centrifugal force of the wheel deposits slurry on the outer edges of the plate.
I-Type Cracks (8): Unequal drying of the clay body can result in uneven shrinkage forces exceeding the dry strength of the clay. Typically, this type of crack happens when wide flat forms are handbuilt or thrown on the wheel and dry from the top down to the base. Different sections of the form give up water to evaporation at dissimilar rates, resulting in parts that dry first and shrink. This discrepancy creates internal tensile stresses in the clay.
A number of different forces are at work in the drying process. Cracks develop when different parts of the piece dry at different times, resulting in different rates of shrinkage. As water leaves the clay surfaces first the clay platelets move closer together. Thin sections and rims or exposed edges are subject to air movement and dry ahead of thick interior sections, which restrain the dryer areas. Cracks develop when the clay’s tensile stress exceeds the clay’s limits. Many potters confuse slow drying with even drying. Covering the ware in plastic for long periods might induce even drying. However, rotating or flipping the ware on a regular basis might produce even and fast drying.
Conical Cracks (Lime Pop) (9): A round or semi-circular localized crack can develop when a nodule of plaster (gypsum) gets embedded in the moist clay, either from a bat or wedging table. At the bottom of the hole is a white or black speck. The failure occurs due to differential expansion caused by different rates of movement between the clay and plaster. During drying or firing, the clay shrinks around the non-shrinking plaster, causing tensile stresses at the clay/plaster interface.
Bisque Firing Cracks (10): Heating the pots too fast through the 212–1063°F (100–573°C) region can expose the ware to fast removal of mechanical water, chemical water, and quartz inversion, the last of which can cause thermal stress cracking if heated or cooled too fast through the quartz inversion region resulting in dunting, a structural failure where a crack travels entirely through the clay body.
Quartz inversion occurs in the body with silica quartz expanding in volume suddenly at the same time that shrinkage occurs. A reverse of this process happens upon cooling. Any one or combinations of these heating extremes can result in sharp cracks in the pots.
Crack Facts
The widest part of a crack is where it starts.
Frayed edges on a crack indicate it slowly formed when the clay was drying.
A sharp-edge crack can develop during the bisque firing.
An old potters’ saying is, “Cracks stay the same or get worse.”
A clay body with low dry strength is more easily cracked when handled.
Not all cracks start on the surface; some originate internally.
Cracks can expand and grow larger as the clay dries or in the bisque firing.
the author Jeff Zamek started his career 50 years ago. He obtained BFA/MFA degrees in ceramics from Alfred University, College of Ceramics, New York. In 1980, he started Ceramics Consulting Services, a ceramics-consulting firm developing clay body and glaze formulas for ceramics supply companies throughout the US. His books, The Potter’s Studio Clay & Glaze Handbook, What Every Potter Should Know, Safety in the Ceramics Studio, and The Potter’s Health & Safety Questionnaire are available from Jeff Zamek/Ceramics Consulting Services. For technical information, visit www.jeffzamek.com.
1 W.G. Lawrence, Ceramic Science of the Potter. Chilton Book Company, 1972, page 38. 2 W.D. Kingery, H.K. Bowen, Donald R. Uhlmann, Introduction to Ceramics 1st edition, John Wiley & Sons, Inc., New York, pp. 783, 791, 797. 3 Kingery & Francl, “Fundamental Study of Clay: xiii, Drying Behavior & Plastic Properties.”Journal of the American Ceramic Society, Volume 37, 1954, pp. 596–602. 4 W.D. Kingery, H.K Bowen, Donald R. Uhlmann, Introduction to Ceramics, 2nd Edition. 1976. 5 Mizutani, K., Tanisiki, M., Tanaka, Y., and Ido, M., “Materials Removals in Cutting of Ceramics: Fracture Mechanics on Crack Trajectory Due to Large Scale Fracture. “Journal of the Japan Society of Precision Engineering, 49 (4), 1983, pp. 435–440.
Acknowledgements: Jim Fineman Richard Alfred Richard Buncamper
Parts of the article were excerpted from Ceramic Questions & Answers by Jeff Zamek, www.jeffzamek.com, which details a comprehensive list of round-edge and sharp-edge cracks.
We understand your email address is private. You will receive emails and newsletters from Ceramic Arts Network. We will never share your information except as outlined in our privacy policy. You can unsubscribe at any time.
Please enjoy this complimentary article for the month.
For unlimited access to Ceramics Monthly premium content, please subscribe.
We understand your email address is private. You will receive emails and newsletters from Ceramic Arts Network. We will never share your information except as outlined in our privacy policy. You can unsubscribe at any time.
Subscribe to Ceramics Monthly
Cracks tell a story, and if you pay attention to what they are saying, you can troubleshoot your drying and firing problems. While cracks can occur in clay bodies and in glazes, let’s first take a look at clay-body cracks.
Defining the Terms
Bone Dry: Clay that is dry to the touch but still has minimal amounts of mechanical and chemical water. It has no plasticity and is at its weakest point.
Clay Body: A combination of clay(s), fluxes, and fillers to achieve a specific firing range, forming method, fired color, and kiln atmosphere.
Clay Platelets: Microscopic, flat, hexagonal clay plates that, when combined with water, achieve plasticity. The ratio of the long dimension to the plate thickness is approximately 10 to 1. Clay platelets can range in size from 100 microns to 0.1 micron average particle dilatometer.1 (1 micron = 1 millionth of a meter).
Dry Strength: The capacity of clay in the dry state to resist cracking, breaking, or deformation when subjected to stress.
Leather Hard: Clay that is firm but pliable and has enough moisture to be manipulated in a forming process and has not reached the brittle stage in drying. It can be trimmed and supports its own shape.
Quartz Inversion: A reversible transition occurring in the crystalline structure of quartz at approximately 1063°F (533°C), resulting in a sudden change in volume and expansion/contraction.
Tensile Stress: The internal resisting force in a cross section of a material when subjected to pulling forces. Clay is weak in tensile loads and strong in compressive loads.
Thermal Expansion: Increase in the size of ceramic material caused by an increase in temperature.
What Exactly Is a Crack?
A crack occurs when a clay body splits apart internally, indicating a stress overload exceeding its strength, such as uneven shrinkage in drying or firing, high tensile loads, and rapid heating or cooling. This dynamic mechanism (movement of clay particles in response to a force acting on it) also applies to cracks in glazes.
As pottery was produced on a larger commercial scale, a method of crack identification was required. This system offered a standardized pathway to solving cracks.2
When observing a crack, it might be useful to ask the following:
Round-Edge and Sharp-Edge Cracks (1, 2)
The first step in solving a crack defect is to determine if it’s a sharp-edge crack (imagine you hit the fired pot with a hammer) or a round-edge crack (fired glaze rolls back from the edge of the crack). The correct diagnosis at this point is critical.
Round-edge cracks start either in the clay-body formula, forming, drying, or bisque firing stages, and then the glaze was applied over the existing crack. Some round-edge cracks are difficult to observe in leather-hard, bone-dry, or bisque stages. However, when in doubt, run a slightly damp sponge over the suspect areas. Moisture will collect in the crack, making it visible. These cracks will have a round edge as opposed to a sharp hairline fault when fired.
Factors Producing Round-Edge Cracks
Incorrect Clay Body: Often the incorrect clay body is the first suspect in producing a crack. Some clay-body formulas are more likely to crack than others, caused by either end of their plasticity spectrum. Specifically, short clay bodies (low plasticity) can break or tear when subjected to forming stresses, resulting in cracking upon drying. An extremely plastic clay body can have high percentages of fine-grained clays such as ball clays or bentonite. These clays have a high water state for plasticity, causing excessive shrinkage and cracking upon drying. Conversely, clay bodies with small, medium, and largeplatelet sizes can increase packing within the structure, which reduces shrinking and drying cracks. An important first step in preventing potential cracks is to choose the appropriate clay body for the forming method.
Shrinkage (3): Different rates of shrinkage in drying or bisque firing can cause stress cracks in several ways. The use of two or more different clay bodies can induce cracking in drying or bisque firing due to different shrinkage rates exceeding the clays’ ability to withstand tensile stress. During a firing, each clay can have different rates of thermal expansion in heating and cooling, leading to a failure.
When a dry piece of clay is attached to another piece, and as the two exhibit different shrinkage rates in drying or bisque firing, a crack, or a semi-dry clay face with small movable unstable particles interrupts the joined surface, it acts as a parting layer between the two assembled sections.3
Cracks can result when thin sections are joined to thicker sections of clay. Thin sections of clay dry quickly and begin to shrink, while thicker sections of clay containing water have not begun to shrink at an equivalent rate.
Bone-Dry Clay Breakage (4): Bone-dry pots, brittle and lacking moisture, are at their weakest state. The clay platelets are tightly packed but with little or no free water film to bind them weakly together. The pot may not appear to be cracked, but cracks can develop in the later stages of forming or drying. At the point of impact, compressive stress is generated while producing tensile stress on the opposite side of the impact. Tensile stress is greater than the clay’s ability to withstand the impact, forming micro-cracks which can propagate.4
Trimming Crack (5): The tip of the trim tool applies compressive pressure as it comes in contact with the clay’s surface, causing shear and tensile stresses. The bone-dry or semi-moist clay plus the pressure from the trimming tool are enough to stress the clay and exceed its dry strength. This type of crack happens around the outer or inner circumference of a pot’s foot and can spread as the pot dries, further extending from the original weak point. The less water contained in the pot, the more likely this type of crack will develop.5
S-Type Cracks (6): This frequent type of crack in wheel-thrown pottery is noticed upon the clay’s drying. Centered clay should be thoroughly compressed on the bottom of the form before pulling up the walls. A more effective approach is, after centering the clay, to pull it up into a cylinder shape, then compress it onto the bat. This aligns the clay platelets and prevents S-type cracks. Shallow elongated S-type cracks can sometimes occur in slab-built or wheel-thrown forms due to not wedging the clay before forming.
O- and C-Type Cracks (7): As the name implies, cracks are circular and frequently appear in the drying stage. They are caused by excess water or slurry (a clay/water mixture) being left in the ware. Cracks are frequently seen in the outer rims of thrown plates where the slurry mixture has been thrown by the centrifugal force of the wheel. Often the slurry is difficult to distinguish from the surrounding clay. The same process occurs at the bottom inner edge of a thrown cylinder where the slurry has not been removed. O-type cracks occur when the centrifugal force of the wheel deposits slurry on the outer edges of the plate.
I-Type Cracks (8): Unequal drying of the clay body can result in uneven shrinkage forces exceeding the dry strength of the clay. Typically, this type of crack happens when wide flat forms are handbuilt or thrown on the wheel and dry from the top down to the base. Different sections of the form give up water to evaporation at dissimilar rates, resulting in parts that dry first and shrink. This discrepancy creates internal tensile stresses in the clay.
A number of different forces are at work in the drying process. Cracks develop when different parts of the piece dry at different times, resulting in different rates of shrinkage. As water leaves the clay surfaces first the clay platelets move closer together. Thin sections and rims or exposed edges are subject to air movement and dry ahead of thick interior sections, which restrain the dryer areas. Cracks develop when the clay’s tensile stress exceeds the clay’s limits. Many potters confuse slow drying with even drying. Covering the ware in plastic for long periods might induce even drying. However, rotating or flipping the ware on a regular basis might produce even and fast drying.
Conical Cracks (Lime Pop) (9): A round or semi-circular localized crack can develop when a nodule of plaster (gypsum) gets embedded in the moist clay, either from a bat or wedging table. At the bottom of the hole is a white or black speck. The failure occurs due to differential expansion caused by different rates of movement between the clay and plaster. During drying or firing, the clay shrinks around the non-shrinking plaster, causing tensile stresses at the clay/plaster interface.
Bisque Firing Cracks (10): Heating the pots too fast through the 212–1063°F (100–573°C) region can expose the ware to fast removal of mechanical water, chemical water, and quartz inversion, the last of which can cause thermal stress cracking if heated or cooled too fast through the quartz inversion region resulting in dunting, a structural failure where a crack travels entirely through the clay body.
Quartz inversion occurs in the body with silica quartz expanding in volume suddenly at the same time that shrinkage occurs. A reverse of this process happens upon cooling. Any one or combinations of these heating extremes can result in sharp cracks in the pots.
Crack Facts
the author Jeff Zamek started his career 50 years ago. He obtained BFA/MFA degrees in ceramics from Alfred University, College of Ceramics, New York. In 1980, he started Ceramics Consulting Services, a ceramics-consulting firm developing clay body and glaze formulas for ceramics supply companies throughout the US. His books, The Potter’s Studio Clay & Glaze Handbook, What Every Potter Should Know, Safety in the Ceramics Studio, and The Potter’s Health & Safety Questionnaire are available from Jeff Zamek/Ceramics Consulting Services. For technical information, visit www.jeffzamek.com.
1 W.G. Lawrence, Ceramic Science of the Potter. Chilton Book Company, 1972, page 38.
2 W.D. Kingery, H.K. Bowen, Donald R. Uhlmann, Introduction to Ceramics 1st edition, John Wiley & Sons, Inc., New York, pp. 783, 791, 797.
3 Kingery & Francl, “Fundamental Study of Clay: xiii, Drying Behavior & Plastic Properties.”Journal of the American Ceramic Society, Volume 37, 1954, pp. 596–602.
4 W.D. Kingery, H.K Bowen, Donald R. Uhlmann, Introduction to Ceramics, 2nd Edition. 1976.
5 Mizutani, K., Tanisiki, M., Tanaka, Y., and Ido, M., “Materials Removals in Cutting of Ceramics: Fracture Mechanics on Crack Trajectory Due to Large Scale Fracture. “Journal of the Japan Society of Precision Engineering, 49 (4), 1983, pp. 435–440.
Acknowledgements:
Jim Fineman
Richard Alfred
Richard Buncamper
Parts of the article were excerpted from Ceramic Questions & Answers by Jeff Zamek,
www.jeffzamek.com, which details a comprehensive list of round-edge and sharp-edge cracks.
December 2026: Table of Contents
Must-Reads from Ceramics Monthly
Unfamiliar with any terms in this article? Browse our glossary of pottery terms!
Click the cover image to return to the Table of Contents