The audio file for this article was produced by the Ceramic Arts Network staff and not read by the author.

Maegan June Collins’ set of quilted teacups, slip-cast porcelain.

Fabric can be folded, pleated, stretched, and gathered—and so can clay. These shared material properties sparked my initial interest in creating a sewn-and-slip-cast vessel. 

Inspiration for these quilted vessels came from familiar everyday objects: a puffer coat, the stitching on a duvet, and the wrinkle of a rolled-up sleeve. I was drawn to the way these objects convey movement through gentle folds and subtle textures. At the same time, I became increasingly drawn to geometry and repetition after being introduced to sashiko, a traditional Japanese needlework technique that showcases patterns through a repeated running stitch. The rhythmic repetition found in sashiko, alongside the intricate patterns of traditional ceramic wall tiles, became a significant source of inspiration for the geometric paneling of my quilted vessels.

1 Sketches of different pattern variations for the flower vase. 2 The paper template used for the nylon fabric panels.

Design

This series of ceramic quilted vessels explores the relationship between clay and fabric through techniques of sewing, mold making, and slip-casting. Transforming a textile object into clay requires careful consideration of how the fabric’s structure and surface will transition into a ceramic vessel. I begin by sewing a quilted form, which serves as the positive for a plaster mold. The plaster captures the exterior surface of the textile, creating a negative impression. Porcelain slip is then cast into this negative mold, creating a new ceramic positive that replicates the original textile. My latest piece in this series, a tall cylindrical flower vase, continues this exploration.

3 Drawing the diamond motif onto the nylon. 4 Nylon quilted panels being sewn together.

Sewing 

The process of hand sewing a quilted form involves several steps. First, I sketch the vessel to analyze different heights, widths, and quilted motifs (1). I then create several small-scale paper models to test the proportions and overall shape. From these models, I generate a paper template for each panel to establish consistent dimensions that will maintain the symmetry of the vessel (2). 

5 Flat lay of the nylon panels fully sewn together. 6 Sewing together quilted panels.

Using the template, I cut individual panels from ripstop nylon and draw the diamond motif by hand (3). Two layers of nylon are sewn together, leaving a small opening for the polyester fill (4). Once the panels are filled and closed, I sew the diamond pattern across the surface, compressing the fill into a series of raised and recessed surfaces (5). This process is repeated for each panel before they are sewn together, piece by piece, into a three-dimensional vessel (6). At this stage, the object exists entirely as a soft textile form, but it already contains the shape, structure, and surface pattern that will eventually be expressed in clay (7). 

7 Completed textile form. 8 Textile form being prepared for the mold with clay boundaries.

Mold Making 

Since the quilted form contains subtle undercuts, the mold must be carefully planned to ensure that the cast vase can be released without damage. Early molds resulted in frequent tears and holes, particularly along the stitched seams. These thinner areas became natural pathways for cracks to appear in the clay. Through repeated testing, I was able to reduce these accidents by adjusting my slip recipe, increasing casting times, and dividing the mold into additional sections to reduce stress during removal. 

9 Cottle boards are set up and ready for plaster to be poured. 10 The first section of plaster mold has been poured.

The mold-making process begins by preparing the quilted form. Since the fabric itself is too lightweight and flexible to withstand the weight of the plaster, I insert an internal structure to give the form enough rigidity to hold its shape (8). Once it’s in place within the cottle boards (9), I block off sections with clay to establish the mold boundaries. I then lightly coat the surface of the nylon with mold release to facilitate its removal from plaster later on. I pour the plaster in three stages (10–12) to create multiple sections; this ensures the mold can be gradually opened once cast. As the plaster is poured, it captures the exterior surface of the quilt and produces a negative impression. 

Once the plaster has set, I carefully remove the quilted form and its internal structure from the mold. Then I clean the three sections of the plaster mold, removing any sharp edges and stray fibers, and leave them to dry completely before casting (13).

11 Two sections of the plaster mold are complete. The bottom keys are carved out and prepared for the final pour of plaster. 12 All three sections of plaster have been poured and left to set up.

Slip Casting and Firing

Using porcelain slip, I cast each vase for 20–30 minutes before pouring out the excess. Once the cast has set, I clean up the rim and leave the vase in the mold for 24 hours, allowing the porcelain to reach a soft-leather-hard state. This ensures that the vase is solid enough to hold its shape while remaining pliable enough for careful removal.

13 The three sections of plaster are removed and set aside to dry for a week. 14 Removal of the cast porcelain vase.

The removal process is slow and gentle, and it’s the most rewarding part of the making process for me. Because of the fabric’s subtle undercuts, the mold must be opened gradually to prevent accidental rips. I sometimes partially open the mold and wait an additional hour for the porcelain to firm up before continuing the removal (14). Each time I remove a vase, I witness the transformation of the object I sewed by hand as it reappears in clay, carrying with it an extraordinary amount of surface detail. The plaster captures the tiny stitches and seam lines of the original fabric; even the fine grid of the ripstop nylon is preserved.

15 Cleaning up the seam lines and imperfections of the vase. 16 A clear glaze is applied to the interior of the quilted vessel.

After the vase is successfully removed from the mold, I refine the seam lines and minor imperfections using a curved carving tool, a soft brush, and a sponge (15). The vase is then bisque fired. Afterward, I apply a clear glaze to the interior (16) before firing to cone 6 in an electric kiln. The exterior is left unglazed to preserve the natural surface of the porcelain, allowing light and shadow to emphasize the curves and stretches of the original textile form. Finally, I apply a clear, neutral wax as a surface treatment for the vase to help prevent staining from flowers, pollen, and soil.

Maegan June Collins’ two quilted flower vases and a teacup, 2026. Photo: Audrey Demers. Maegan June Collins’ finished ceramic quilted flower vase.

Finished Vessel

The resulting vessel is a ceramic object that appears soft, reproducing the quilted surface from which it was formed. This illusion creates a surprising tactile response that subverts expectations of ceramic surfaces, inviting the viewer to question the relationship between material and appearance.

For me, this work exists in a space between ceramics and textiles. It is an exploration of how one material can borrow the language of another and how traditional handcraft techniques can be reimagined through contemporary ceramic processes. Most importantly, it invites a reconsideration of clay, not as inherently rigid but as a material capable of capturing softness, movement, and the familiar textures of everyday life.

the author Maegan June Collins is a Taiwanese-Canadian ceramic artist originally from Toronto, Ontario, Canada. She studied ceramics at The Kootenay School of Art in 2021 and is currently practicing out of Montréal, Quebec.

 

Previous December Issue Article                    Next December Issue Article

 

December 2026: Table of Contents


Must-Reads from Ceramics Monthly

Unfamiliar with any terms in this article? Browse our glossary of pottery terms!
Click the cover image to return to the Table of Contents