Creating a Colored Clay 

Use any stain you like to make a strong, saturated color, adding at least 5% stain (calculated based on the weight of the clay). I use wet porcelain from the bag. Make a depression in the ball of clay with your thumb. Add the stain to this well along with a few drops of water to dissolve the stain, and mix it thoroughly between your hands (gloves are recommended for direct handling of metallic stains). I always mix in the wet stain initially with a fork, pulling the sides of the clay into the center to cover the stain, preventing it from going all over my hands and therefore being wasted. 

Weigh the colored clay you’ve just made and match it with the same weight of uncolored clay from the bag. Roll both pieces out so they are identical in length and thickness (1). 

1 Roll stained clay and porcelain into coils of the same thickness and length.

Combining the Clays for Gradients 

With the two coils side by side, carefully measure and cut graduated lengths across both pieces (2). In this example, I started with a 3-mm slice and increased each cut by about 1.5 mm (to be 4.5 mm long), then 1.6 mm (to be 6.1 mm long), then 1.7 mm (to be 7.8 mm long), etc. 

2 Cut the coils into graduated segments.

Working from the end of the colored roll with smaller cuts, pick up the end piece and stick it to the largest section at the opposite end of the white clay roll. Continue placing the colored pieces onto the white pieces until the largest colored piece now has the smallest white piece on top of it (3). 

Each of these pieces now needs to be mixed in turn and placed back down, keeping them in the right sequence (see 4). The clay dries out quickly during this process, so have a damp cotton sheet nearby to place the pieces on and cover them up as you go. 

3 Pair the longest segment of the colored clay with the shortest segment of the white porcelain. Continue matching the segments in reverse order.

4 Blend each pair of colored-clay and white-porcelain segments. Be sure to keep the blended pieces in the correct sequence.

Laminating Clay 

Once the mixing is complete, roll out each piece of blended clay to about 2 mm thickness (5). Dampen each disk lightly with a brush of water and lay the next disk on top. Roll and stack each piece in sequence until finished (6). Tip: When laminating clay, always lay the piece down from left to right so that air is not captured between the layers. 

5 Use a pony roller to roll each blended piece into a 2-mm-thick disk. 6 Stack the disks in order, sticking them together with a small amount of water.

The finished stack should now look like it is going from the lightest shade to the darkest. Cut the stack in half to reveal the graduation (7). The block can now be used by slicing and rearranging as you please. 

7 Cut the stack in half to reveal the gradual blend.

This article originally appeared in Ceramics Monthly in January 2022. 

Anne Mossman was an Australian-based potter, who passed away in 2024. Her porcelain vessels were made using the nerikomi method. You can find many of her pots and techniques on Instagram @annemossman. 

 

 

November/December 2025: Table of Contents


Must-Reads from Pottery Making Illustrated

Unfamiliar with any terms in this article? Browse our glossary of pottery terms!
Click the cover image to return to the Table of Contents