Naomi Peterson loves the meditative process of making intricately detailed work. Yet, when she wanted to experiment with more color and pattern on her surfaces, she quickly realized she needed a more streamlined process. Enter sprig molds.
In this post, an excerpt from the Pottery Making Illustrated archive, Naomi walks you through the process of creating sprig molds from positives. If you're ready to experiment with textured surfaces, this technique will open up a world of possibilities in your ceramic practice. Ready to work smarter, not harder? Read on! - Jennifer Poellot Harnetty, editor
I have always been a fan of extremely finicky and time-consuming processes; through slow-paced studio days, I can work through forms intuitively and meditate on ideas for hours. While this is great for coming up with interesting constructions, it is not
conducive to experimentation in other areas of my studio practice. For instance, during the time post-graduate school, I wanted to incorporate more color and pattern into my pieces, but because of the amount of time it took to construct each individual
attachment (i.e. measuring out, rolling out, and attaching individual balls) that would cover a significant section of a vessel, my progress exploring surface variations was slow and frustrating. I needed a process that would fit the old adage “work
smarter not harder,” so I could have more time for other areas of my studio practice. I wanted a tool that would help me measure, shape, and attach small pieces of clay all in one. A small press mold or sprig mold was the solution (A).
Positives and Negatives
For the purpose of experimentation and efficiency, I decided to create bisque-fired ceramic positives, with which I could make as many sprig molds as I wanted (B). This way, if the original sprig mold gets lost or damaged, replacements or variations of
the original design can be made faster than trying to recreate the tool from scratch.
A positive is the exact shape and size your sprig will be, so making sure all details are smoothed and preventing undercuts (C) is key to making a successful positive. Using cookie cutters or simple guides is a great way to make a positive. Once you have
a finalized form that you want to make a sprig mold of, attach it to a small slab of clay. Do this at the leather-hard stage to prevent details from getting smudged. I recommend using a simple, round-edged shape to help prevent chips and breaks.
Bisque fire the positive before making the sprig mold.
Creating Sprig Molds Using Positives
To make a sprig mold, roll a small clay ball using soft, fresh clay into a small cone approximately the size of a baby carrot. The fatter end should be smooth, wrinkle-free, and the diameter should be a bit wider than your positive’s form. Position
this fatter end directly above and in the center of the positive, and press down firmly to ensure all details transfer. Set the new sprig mold aside to dry to leather hard, after which you can trim off the excess using a knife, cheese cutter, or loop
tool. Ensure the tapered end where your fingers hold the tool isn’t smooth; a textured handle helps you grip the tool. Bisque fire the sprig mold before use. Takeaways:
Positive/Master Mold: Sculpted form attached to a small slab, bisque fired, representation of what the final sprig will look like. Start simple and build complexity, avoiding all undercuts.
Negative/Sprig Mold: Small press mold made from a positive master mold for creating low-relief shapes. Bisque fired for durability and reuse. The negative space inside is to be filled with clay to create sprigs.
Positive/Sprigs: Sprig molds are used for creating sprigs. Sprigs are pressed clay attached to a clay object’s surface for relief decoration.
Naomi Peterson received an MFA in ceramics from the University of North Texas. In 2024, she was selected as an Emerging Artist by Ceramics Monthly. Naomi has taught nationally at various institutions such as the Glassell School of Art and Art League Houston as well as teaching workshops online and in person. Currently, she is an artist-in-residence at KC Clay Guild.
Search the Daily
Published Aug 12, 2026
Naomi Peterson loves the meditative process of making intricately detailed work. Yet, when she wanted to experiment with more color and pattern on her surfaces, she quickly realized she needed a more streamlined process. Enter sprig molds.
In this post, an excerpt from the Pottery Making Illustrated archive, Naomi walks you through the process of creating sprig molds from positives. If you're ready to experiment with textured surfaces, this technique will open up a world of possibilities in your ceramic practice. Ready to work smarter, not harder? Read on! - Jennifer Poellot Harnetty, editor
PS. See how Naomi uses her sprig molds to spruce up her surfaces in the March/April 2025 issue of Pottery Making Illustrated! Not a subscriber? Subscribe today!
I have always been a fan of extremely finicky and time-consuming processes; through slow-paced studio days, I can work through forms intuitively and meditate on ideas for hours. While this is great for coming up with interesting constructions, it is not conducive to experimentation in other areas of my studio practice. For instance, during the time post-graduate school, I wanted to incorporate more color and pattern into my pieces, but because of the amount of time it took to construct each individual attachment (i.e. measuring out, rolling out, and attaching individual balls) that would cover a significant section of a vessel, my progress exploring surface variations was slow and frustrating. I needed a process that would fit the old adage “work smarter not harder,” so I could have more time for other areas of my studio practice. I wanted a tool that would help me measure, shape, and attach small pieces of clay all in one. A small press mold or sprig mold was the solution (A).
Positives and Negatives
For the purpose of experimentation and efficiency, I decided to create bisque-fired ceramic positives, with which I could make as many sprig molds as I wanted (B). This way, if the original sprig mold gets lost or damaged, replacements or variations of the original design can be made faster than trying to recreate the tool from scratch.
A positive is the exact shape and size your sprig will be, so making sure all details are smoothed and preventing undercuts (C) is key to making a successful positive. Using cookie cutters or simple guides is a great way to make a positive. Once you have a finalized form that you want to make a sprig mold of, attach it to a small slab of clay. Do this at the leather-hard stage to prevent details from getting smudged. I recommend using a simple, round-edged shape to help prevent chips and breaks. Bisque fire the positive before making the sprig mold.
Creating Sprig Molds Using Positives
To make a sprig mold, roll a small clay ball using soft, fresh clay into a small cone approximately the size of a baby carrot. The fatter end should be smooth, wrinkle-free, and the diameter should be a bit wider than your positive’s form. Position this fatter end directly above and in the center of the positive, and press down firmly to ensure all details transfer. Set the new sprig mold aside to dry to leather hard, after which you can trim off the excess using a knife, cheese cutter, or loop tool. Ensure the tapered end where your fingers hold the tool isn’t smooth; a textured handle helps you grip the tool. Bisque fire the sprig mold before use. Takeaways:
Naomi Peterson received an MFA in ceramics from the University of North Texas. In 2024, she was selected as an Emerging Artist by Ceramics Monthly. Naomi has taught nationally at various institutions such as the Glassell School of Art and Art League Houston as well as teaching workshops online and in person. Currently, she is an artist-in-residence at KC Clay Guild.
**First published in 2025.
Unfamiliar with any terms in this article? Browse our glossary of pottery terms!
Related Content
Ceramic Artists
Functional Pottery
Ceramic Sculpture
Glaze Chemistry
High-Fire Glaze Recipes
Mid-Range Glaze Recipes
Low-Fire Glaze Recipes
Ceramic Colorants
Ceramic Glazes and Underglazes
Ceramic Raw Materials
Pottery Clay
Ceramic Decorating Tools
Ceramic Kilns
Making Clay Tools
Wheel Throwing Tools
Electric Kiln Firing
Gas Kiln Firing
Raku Firing
Salt Firing and Soda Firing
Wood Kiln Firing
Ceramic Decorating Techniques
Ceramic Glazing Techniques
Handbuilding Techniques
Making Ceramic Molds
Making Ceramic Tile
Wheel Throwing Techniques