To get the most out of commercial ceramic glazes in your electric kiln, you need to understand the product descriptions on the package. What do the manufacturers mean when they say opaque, semi transparent, or translucent? Do their descriptions match the descriptions in your head? Of course, the best way to find this out is to test, test, test!
In this post, an excerpt from Off the Shelf | Outside the Box, Deklan Ranlett has done some of that testing legwork for you and shares the results of testing some commercial ceramic glazes over texture in their electric kiln. - Jennifer Poellot Harnetty, editor
Part of navigating the use of commercial glazes is understanding the phraseology on the jar. Most glaze manufacturers use terms such as opaque, semi-translucent, translucent, transparent, etc., on their labels. But what do those words really mean? How would each affect the surface if you like to sgraffito, add thick slip, use sprigs, carve, or stamp? To answer this question, I designed a test tile with a little of each of these techniques to test cone 04 and cone 6 commercial glazes and to illustrate some important factors to consider when using these glazes.
The test tiles included: sgraffito using Amaco’s LUG-1 Black Underglaze; dots of white slip made with Little Loafers and 5% Zircopax; an incised diagonal pattern; gemstone-shaped sprigs from plaster molds; a row of stamps; and finally a water-etching. It’s important to make a test bar of your desired texture techniques to use when trying out new glazes so you don’t expect one thing from reading the label or looking at a small tile and get a result you aren’t happy with.
I followed the manufacturer’s directions and brushed three coats of glaze on each tile with a soft fan brush, then glaze fired the tiles to cone 04 or cone 6.
Opaque Ceramic Glazes
Opaque means not letting light through: not transparent.
Tile #1 Mayco Olive Green FN-021, fired to cone 04: The glaze creates a thick layer of color, almost as if the tile has been coated in paint or dipped into colored rubber. The glaze flows into the incised lines and stamps, and there are only breaks in the glaze where the texture is deep. Even the black underglaze is obscured. This glaze would be ideal if you needed very solid coverage.
Tile #3 Mayco Copper Float SW-129, fired to cone 6: The glaze creates a thick layer of color and added sparkle with copper-like flecks. It has a very interactive surface while being opaque—meaning that all opaque glazes are not alike. This glaze shows a lot more of the texture and highlights the deeper lines while interacting with the black underglaze to create a deep, shimmery black in that area.
Semi-Transparent Ceramic Glazes
Semi-transparent means partially or imperfectly transparent.
Tile #4 Amaco Robin’s Egg TP-26, fired to cone 04: The glaze is capable of showing a break over deeper stamped and water-etched textures, shows a slight break on the gemstone sprigs, and gives highlights on the slip-trailed dots. However, it’s very cloudy over the black underglaze—not showing much of the black, so it wouldn’t be a good choice for sgraffito work.
Tile #6 Mayco Green Opal SW-253, fired to cone 6: This glaze creates pools of frothy spring green and, while the glaze fills in some of the texture and incised lines, it acts to highlight breaks over texture and slip trailing and also shows the black underglaze very well in the sgraffitoed areas.
Translucent/Transparent Ceramic Glazes
Translucent means clear or allowing light to pass through. This type of glaze is perfect for highlighting fine details.
Tile #8 Mayco Sky Diamonds CG-975, fired to cone 04: The glaze is showing off each texture to its full advantage, you can see the black underglaze very well and you can also see every facet of the gemstone sprig. It’s worth noting that the physical larger crystal granules you see when applying this glaze pop and pool during firing and you can lose details in those areas. The crystals are the blue and white dots scattered across the fired surface of the tile. You can control this effect to some extent by placing the crystals where you want them when you’re brushing on the glaze.
Tile #10 Mayco Turquoise SW-201, fired to cone 6: This glaze highlights the textures on the tile, isn’t quite as transparent as the Amaco celadon, but still a lovely glaze to use over a variety of textures. The black underglaze is particularly pretty with the turquoise over it.
Deklan Ranlett owns MudFire in Decatur, Georgia (www.mudfire.com).
Search the Daily
Published Nov 28, 2023
To get the most out of commercial ceramic glazes in your electric kiln, you need to understand the product descriptions on the package. What do the manufacturers mean when they say opaque, semi transparent, or translucent? Do their descriptions match the descriptions in your head? Of course, the best way to find this out is to test, test, test!
In this post, an excerpt from Off the Shelf | Outside the Box, Deklan Ranlett has done some of that testing legwork for you and shares the results of testing some commercial ceramic glazes over texture in their electric kiln. - Jennifer Poellot Harnetty, editor
Part of navigating the use of commercial glazes is understanding the phraseology on the jar. Most glaze manufacturers use terms such as opaque, semi-translucent, translucent, transparent, etc., on their labels. But what do those words really mean? How would each affect the surface if you like to sgraffito, add thick slip, use sprigs, carve, or stamp? To answer this question, I designed a test tile with a little of each of these techniques to test cone 04 and cone 6 commercial glazes and to illustrate some important factors to consider when using these glazes.
The test tiles included: sgraffito using Amaco’s LUG-1 Black Underglaze; dots of white slip made with Little Loafers and 5% Zircopax; an incised diagonal pattern; gemstone-shaped sprigs from plaster molds; a row of stamps; and finally a water-etching. It’s important to make a test bar of your desired texture techniques to use when trying out new glazes so you don’t expect one thing from reading the label or looking at a small tile and get a result you aren’t happy with.
I followed the manufacturer’s directions and brushed three coats of glaze on each tile with a soft fan brush, then glaze fired the tiles to cone 04 or cone 6.
Opaque Ceramic Glazes
Opaque means not letting light through: not transparent.Tile #1 Mayco Olive Green FN-021, fired to cone 04: The glaze creates a thick layer of color, almost as if the tile has been coated in paint or dipped into colored rubber. The glaze flows into the incised lines and stamps, and there are only breaks in the glaze where the texture is deep. Even the black underglaze is obscured. This glaze would be ideal if you needed very solid coverage.
Tile #3 Mayco Copper Float SW-129, fired to cone 6: The glaze creates a thick layer of color and added sparkle with copper-like flecks. It has a very interactive surface while being opaque—meaning that all opaque glazes are not alike. This glaze shows a lot more of the texture and highlights the deeper lines while interacting with the black underglaze to create a deep, shimmery black in that area.
Semi-Transparent Ceramic Glazes
Semi-transparent means partially or imperfectly transparent.Tile #4 Amaco Robin’s Egg TP-26, fired to cone 04: The glaze is capable of showing a break over deeper stamped and water-etched textures, shows a slight break on the gemstone sprigs, and gives highlights on the slip-trailed dots. However, it’s very cloudy over the black underglaze—not showing much of the black, so it wouldn’t be a good choice for sgraffito work.
Tile #6 Mayco Green Opal SW-253, fired to cone 6: This glaze creates pools of frothy spring green and, while the glaze fills in some of the texture and incised lines, it acts to highlight breaks over texture and slip trailing and also shows the black underglaze very well in the sgraffitoed areas.
Translucent/Transparent Ceramic Glazes
Translucent means clear or allowing light to pass through. This type of glaze is perfect for highlighting fine details.Tile #8 Mayco Sky Diamonds CG-975, fired to cone 04: The glaze is showing off each texture to its full advantage, you can see the black underglaze very well and you can also see every facet of the gemstone sprig. It’s worth noting that the physical larger crystal granules you see when applying this glaze pop and pool during firing and you can lose details in those areas. The crystals are the blue and white dots scattered across the fired surface of the tile. You can control this effect to some extent by placing the crystals where you want them when you’re brushing on the glaze.
Tile #10 Mayco Turquoise SW-201, fired to cone 6: This glaze highlights the textures on the tile, isn’t quite as transparent as the Amaco celadon, but still a lovely glaze to use over a variety of textures. The black underglaze is particularly pretty with the turquoise over it.
Deklan Ranlett owns MudFire in Decatur, Georgia (www.mudfire.com).
Want more information? Check out these articles for information about slow cooling and cone 6 glazes.
**First published in 2015.
Unfamiliar with any terms in this article? Browse our glossary of pottery terms!
Related Content
Ceramic Artists
Functional Pottery
Ceramic Sculpture
Glaze Chemistry
High-Fire Glaze Recipes
Mid-Range Glaze Recipes
Low-Fire Glaze Recipes
Ceramic Colorants
Ceramic Glazes and Underglazes
Ceramic Raw Materials
Pottery Clay
Ceramic Decorating Tools
Ceramic Kilns
Making Clay Tools
Wheel Throwing Tools
Electric Kiln Firing
Gas Kiln Firing
Raku Firing
Salt Firing and Soda Firing
Wood Kiln Firing
Ceramic Decorating Techniques
Ceramic Glazing Techniques
Handbuilding Techniques
Making Ceramic Molds
Making Ceramic Tile
Wheel Throwing Techniques