All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 14.00
Dolomite 12.00
Wollastonite 10.00
Ferro Frit 3124 8.00
Cornwall Stone 46.00
EPK Kaolin 10.00
Add Amount
Zircopax 10.00

Instructions


Opaque gloss glaze that works well for inlaying into textured areas.

This recipe was shared by Kelly Justice in the March/April 2019 issue of Pottery Making Illustrated.