Microwave Kilns: Great Tools for Testing Low-Fire Lusters, Enamels, and China Paints
Microwave kilns are a quick and easy way to get near instant results!
Jessica Knapp
Many people know that a microwave oven can be used to dry clay quickly when you’re in a pinch. Dielectric heating (the type used in a microwave oven) is also used in industry to fire ceramics for high-tech applications. This option is also available on a small scale to the studio potter, at least for firing tests and small objects using a microwave kiln.
While the kilns don't fire high enough to test higher temperature glazes or clay bodies, they can really help out if you are interested in low-fire decorative applications such as china paints, lusters, egyptian paste, overglaze enamels and many commercial decals. In this post, Jessica Knapp tells you all about this alternate use for old microwaves! - Jennifer Poellot Harnetty, editor.
A microwave kiln is a container kiln consisting of a base and hood made for use in a household microwave oven. The kiln is made of a white insulating fiber and lined on the inside of the chamber with a black compound that absorbs the microwave radiation
and heats up to 1650°F or approximately cone 010 (figure A). The heat from this compound is then transferred to the chamber and to the piece being fired. It takes between 5 to 10 minutes to reach peak temperature ranges depending on the size of the
microwave kiln, the work being fired, and the microwave’s wattage. After the firing, the kiln needs to cool for at least 20 minutes before being opened.
Designed for working primarily with small glass objects or precious metal clay, the microwave kiln is also suitable for firing small clay pieces, from beads and pendants to test tiles or small sculptural objects. The kilns come in three sizes. The small
and medium size have a firing chamber that’s 1¾ inches in height, and a diameter of 2¾ inches and 4½ inches respectively. The chamber in the large kiln measures 61/4 inches in diameter by 23/8 inches high.
The optimum firing time for various materials and sizes needs to be determined through test firings. Spectrum Glazes, one of the kiln’s distributors, sells a range of glaze pens formulated specifically for the kiln (see figure A) but overglazes, glazes,
and clays formulated for a range between cones 018 and 010 can be successfully fired.
Using the Microwave Kiln
First, cut a piece of kiln fiber paper to size. The fiber paper is usually provided as part of the kit (see figure A), but can be replaced by pieces of Bullseye Thin-Fire paper used for glass work.
The fiber paper prevents anything from sticking to the insulating fiber base.Place your piece on the fiber paper and test fit the cover to be sure the piece does not hit the top or sides of the firing chamber (figure B). Place the base in the microwave
and cover with the lid. Be careful; the black coating on the inside of the lid is delicate and cracks off easily if bumped.
Set the microwave timer based on your tests. Once the microwave turns off, you’ll notice an orange glow coming from the vent hole in the top of the kiln. You do not need to use kiln wash in this kiln. Take the kiln out of the microwave immediately to prevent damage to the microwave’s ceiling from prolonged exposure to the heat from the vent hole. Wearing oven mitts or kiln gloves, grasp both the
top and bottom of the kiln at the same time, taking care to not open it as you lift it up (figure C). Place the kiln on a heat resistant surface, like a brick or tile.
Leave the kiln closed for 20–30 minutes before opening. For slightly larger work, increase the cooling time to 35–40 minutes. The top of the cover and bottom of the base stay very hot for a long
time, so keep at least a 6-inch clearance above and around the kiln. After cooling, gently brush the fiber paper residue off of the base with a soft brush.
Note: Wear a respirator to avoid inhaling the dust.
When using this kiln, follow the same rules as you would when firing work in a larger kiln. Clay objects can be fired either green or after
a bisque firing. If firing green, the work must be thin and dry. Dry glazed work overnight before firing. Due to fumes, the microwave needs to be vented properly or fired outside. Take careful notes. As the microwave kilns are too small to insert
a pyrometer, and, unless you buy the larger model, also too small for a cone pack, you’ll need to take notes on the time/temperature correlation for your own microwave.
Testing your Microwave Kiln
We tested the Spectrum multi pens (figure 1), a white gold and a mother-of-pearl luster, a purple overglaze enamel (figures 2–4), commercial underglazes (figure 5), an 04 transparent glaze, and Egyptian paste. It took additional tests to find the correct
firing time for the enamels and the lusters. The firings for the two overglazes produced noticeably more fumes and discoloration in the kiln than the other glaze firings.
As a general guideline, with a low-powered microwave, it took 3 minutes to fire a piece with luster or overglaze and 5 minutes to fire the glaze pens and underglazes.
For clay bodies, two Egyptian pastes, fired green, a bisque-fired porcelain body, and a high-fired porcelain body. All of the clay bodies survived the thermal shock of the short firings (4 to 5 minutes for the Egyptian paste, and 5 minutes for the
porcelain).
Conclusion
Though it won’t replace your need for a larger kiln, a microwave kiln can help speed up your glaze and clay body testing, or provide a way to make small-scale objects or even models for larger pieces.Microwave kilns are sold under three different brand
names: MicroKiln, MagicFuse, and Fuseworks. Check with your local distributor for availability. All three can also be found online.
A special thank you to Spectrum Glazes (www.spectrumglazes.com) for providing a MicroKiln for use in testing clays and glazes for this article.
Search the Daily
Published Dec 27, 2021
While the kilns don't fire high enough to test higher temperature glazes or clay bodies, they can really help out if you are interested in low-fire decorative applications such as china paints, lusters, egyptian paste, overglaze enamels and many commercial decals. In this post, Jessica Knapp tells you all about this alternate use for old microwaves! - Jennifer Poellot Harnetty, editor.
A microwave kiln is a container kiln consisting of a base and hood made for use in a household microwave oven. The kiln is made of a white insulating fiber and lined on the inside of the chamber with a black compound that absorbs the microwave radiation and heats up to 1650°F or approximately cone 010 (figure A). The heat from this compound is then transferred to the chamber and to the piece being fired. It takes between 5 to 10 minutes to reach peak temperature ranges depending on the size of the microwave kiln, the work being fired, and the microwave’s wattage. After the firing, the kiln needs to cool for at least 20 minutes before being opened.
Designed for working primarily with small glass objects or precious metal clay, the microwave kiln is also suitable for firing small clay pieces, from beads and pendants to test tiles or small sculptural objects. The kilns come in three sizes. The small and medium size have a firing chamber that’s 1¾ inches in height, and a diameter of 2¾ inches and 4½ inches respectively. The chamber in the large kiln measures 61/4 inches in diameter by 23/8 inches high.
The optimum firing time for various materials and sizes needs to be determined through test firings. Spectrum Glazes, one of the kiln’s distributors, sells a range of glaze pens formulated specifically for the kiln (see figure A) but overglazes, glazes, and clays formulated for a range between cones 018 and 010 can be successfully fired.
Using the Microwave Kiln
First, cut a piece of kiln fiber paper to size. The fiber paper is usually provided as part of the kit (see figure A), but can be replaced by pieces of Bullseye Thin-Fire paper used for glass work. The fiber paper prevents anything from sticking to the insulating fiber base.Place your piece on the fiber paper and test fit the cover to be sure the piece does not hit the top or sides of the firing chamber (figure B). Place the base in the microwave and cover with the lid. Be careful; the black coating on the inside of the lid is delicate and cracks off easily if bumped.
Set the microwave timer based on your tests. Once the microwave turns off, you’ll notice an orange glow coming from the vent hole in the top of the kiln. You do not need to use kiln wash in this kiln. Take the kiln out of the microwave immediately to prevent damage to the microwave’s ceiling from prolonged exposure to the heat from the vent hole. Wearing oven mitts or kiln gloves, grasp both the top and bottom of the kiln at the same time, taking care to not open it as you lift it up (figure C). Place the kiln on a heat resistant surface, like a brick or tile.
Note: Wear a respirator to avoid inhaling the dust.
When using this kiln, follow the same rules as you would when firing work in a larger kiln. Clay objects can be fired either green or after a bisque firing. If firing green, the work must be thin and dry. Dry glazed work overnight before firing. Due to fumes, the microwave needs to be vented properly or fired outside. Take careful notes. As the microwave kilns are too small to insert a pyrometer, and, unless you buy the larger model, also too small for a cone pack, you’ll need to take notes on the time/temperature correlation for your own microwave.
Testing your Microwave Kiln
We tested the Spectrum multi pens (figure 1), a white gold and a mother-of-pearl luster, a purple overglaze enamel (figures 2–4), commercial underglazes (figure 5), an 04 transparent glaze, and Egyptian paste. It took additional tests to find the correct firing time for the enamels and the lusters. The firings for the two overglazes produced noticeably more fumes and discoloration in the kiln than the other glaze firings.
As a general guideline, with a low-powered microwave, it took 3 minutes to fire a piece with luster or overglaze and 5 minutes to fire the glaze pens and underglazes. For clay bodies, two Egyptian pastes, fired green, a bisque-fired porcelain body, and a high-fired porcelain body. All of the clay bodies survived the thermal shock of the short firings (4 to 5 minutes for the Egyptian paste, and 5 minutes for the porcelain).
Conclusion
Though it won’t replace your need for a larger kiln, a microwave kiln can help speed up your glaze and clay body testing, or provide a way to make small-scale objects or even models for larger pieces.Microwave kilns are sold under three different brand names: MicroKiln, MagicFuse, and Fuseworks. Check with your local distributor for availability. All three can also be found online.
A special thank you to Spectrum Glazes (www.spectrumglazes.com) for providing a MicroKiln for use in testing clays and glazes for this article.
**First published in 2010.
Related Content
Ceramic Artists
Functional Pottery
Ceramic Sculpture
Glaze Chemistry
High Fire Glaze Recipes
Mid-Range Glaze Recipes
Low Fire Glaze Recipes
Ceramic Colorants
Ceramic Glazes and Underglazes
Ceramic Raw Materials
Pottery Clay
Ceramic Decorating Tools
Ceramic Kilns
Making Clay Tools
Wheel Throwing Tools
Electric Kiln Firing
Gas Kiln Firing
Raku Firing
Salt Firing and Soda Firing
Wood Kiln Firing
Ceramic Decorating Techniques
Ceramic Glazing Techniques
Handbuilding Techniques
Making Ceramic Molds
Making Ceramic Tile
Wheel Throwing Techniques