All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 1.00
strontium carbonate 20.00
nepheline syenite 60.00
Ball Clay 10.00
silica 9.00
Add Amount
BENTONITE 2.00

Instructions

This is a flexible glaze that does well in both cooler and hotter spots in the kiln. The matte can form some reflective crystals. I love using this glaze together with Amber Celadon for the liveliness arising from the contrast between glossy and matte, warm and cool. 

 

This recipe was shared by Gay Smith in the November 2022 issue of Ceramics Monthly.