All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
talc 10.22
wollastonite 8.88
ferro frit 3134 19.61
custer feldspar 43.52
epk kaolin 8.89
silica 8.88
Add Amount
bentonite 1.88
zircopax 8.15

Instructions

This recipe was shared by Michael Lemke in the May/June 2022 issue of Pottery Making Illustrated.