All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 66.00
Soda Feldspar 17.00
Nepheline Syenite 6.00
EPK Kaolin 11.00
Add Amount
Zircopax 12.00

Instructions

When used in low-temperature soda firings, I mix and apply this glaze to a skim-milk thinness. For electric firings, I apply this glaze to a standard thickness.

 

This recipe was shared by Peter Jadoonath in the December 2024 issue of Ceramics Monthly.