All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
nepheline syenite 30.61
Helmer Kaolin 62.25
silica 7.14
Add Amount
BENTONITE 2.00

Instructions

Apply the slip to a leather-hard surface. Mix to a consistency similar to whole milk/light cream. 

 

This recipe was shared by Paul Wisotzky in the November 2022 issue of Ceramics Monthly.