All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 6.37
EPK Kaolin 46.82
OM 4 Ball Clay 46.81
Add Amount
zircopax 11.37

Instructions

This slip should be applied thinly at the leather hard stage. Works well in wood and soda firings. 

 

This recipe was shared by Ian Bassett in the November 2022 issue of Ceramics Monthly.