All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
gerstley borate 3.25
Whiting 7.50
Wollastonite 14.00
Custer Feldspar 22.00
Alberta Slip 36.00
EPK Kaolin 3.25
silica 14.00
Add Amount
yellow ochre 7.00
BENTONITE 2.00
Wadding Recipe

Instructions

This is a flexible glaze that does well in both cooler and hotter spots in the kiln. It breaks nicely over edges. As the iron content of mined yellow ochre is inconsistent, testing percentage for color is recommended. I love using this glaze together with Pete’s Strontium Matte for the liveliness arising from the contrast between glossy and matte, warm and cool.  

This recipe was shared by Gay Smith in the November 2022 issue of Ceramics Monthly.