All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 24.00
Custer Feldspar 28.00
EPK Kaolin 20.00
Silica 28.00
Add Amount
Zinc Oxide 3.00
Chrome Oxide 0.30
Cobalt Carbonate 1.00

Instructions

This recipe was shared by Caleb Zouhary in "Cone 6–11 Recipes" in the November 2018 issue of Ceramics Monthly.
I use this as the base glaze on my work, and layer one or two glazes over it, including White Salt. I fire this to cone 11.