All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 23.63
Nepheline Syenite 71.55
OM 4 Ball Clay 4.82
Add Amount
Zircopax 17.92
Bentonite 4.50

Instructions


Mix to the consistency of creamer. If applied too thick, this glaze may bubble during the firing. Add a teaspoon of Epsom salt to help with suspension.

This recipe was shared by Lisa York in the April 2020 issue of Ceramics Monthly.