All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 1.00
Strontium Carbonate 20.00
Nepheline Syenite 60.00
Ball Clay 10.00
Silica 9.00
Add Amount
Cobalt Carbonate 1.00
Copper Carbonate 3.00

Instructions

Published in "Mid-Range Mattes" by Holly Goring, in the January 2017 issue of Ceramics Monthly.

This is a very stable and dense satin matte glaze.
This base works well with other colorants. It is brightest on a porcelain or white stoneware clay body.