All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Strontium Carbonate 18.52
Whiting 10.40
Custer Feldspar 59.42
Ball Clay (OM 4) 11.66
Add Amount
Rutile 9.20
Ultrox (substitute Zirconium) 7.70
Bentonite 1.20

Instructions

Published in "Strontium/Barium" by Dave Finkelnburg, inthe Nov 2014 issue of Ceramics Monthly.