All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 1.00
Strontium Carbonate 20.00
Nepheline Syenite 60.00
Ball Clay 10.00
Silica 9.00
Add Amount
Titanium Dioxide 5.00
Copper Carbonate 5.00
Bentonite 2.00

Instructions

This glaze has a wide firing range. It is more bronze like in coloration and depth at cone 9 in reduction. This glaze breaks on the edges and pools in recesses. Attributed to Pete Pinnell.

Published in "Mid-Range Mattes" by Holly Goring, in the January 2017 issue of Ceramics Monthly.