All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 21.00
Whiting 8.00
Nepheline Syenite 30.00
EPK Kaolin 10.00
Silica 31.00
Add Amount
Mason Stain Robin's Egg 6376 2.00

Instructions


*Add colorant for Celadon.

This is a transparent glaze with a light blue tint. Apply a thin layer to avoid crazing. This is an excellent glaze base for adding colorants to create a palette of colors.

This recipe was shared by Ashley Kim in the March/April 2019 issue of Pottery Making Illustrated.