All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 17.00
Whiting 3.00
Custer Feldspar 53.00
EPK Kaolin 27.00
Add Amount
Cobalt Oxide 2.00
Manganese Dioxide 2.00
Mason Stain 6600 3.00
Bentonite 2.00

Instructions

This recipe was shared by Paul Ide in the February 2019 issue of Ceramics Monthly.
This semi-matte, cone 10 glaze also works well at cone 6. Do not use as a liner glaze.