All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
NC 4 Feldspar 12.00
Hawthorne Fireclay 20.00
XX Saggar Ball Clay 16.00
Cedar Heights Goldart 26.00
Helmar Kaolin 12.00
Alumina 6.00
Silica 8.00

Instructions

Published in "Woodfire Glazes" by Matt Schiemann, in the Jan 2014 issue of Ceramics Monthly.
This clay body works well in wood fired kilns. Helmar Kaolin is added to increase the flashing response of the clay when exposed to the wood-kiln atmosphere.