All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 22.00
Whiting 12.00
Potash Feldspar 35.00
China Clay 15.00
Silica 16.00
Add Amount
Copper Oxide 1.00

Instructions

Published in "Cool Colors" by Linda Bloomfield, in the Feb 2012 issue of Ceramics Monthly.