All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 4.44
Lithium Carbonate 2.22
Magnesium Carbonate 25.19
Ferro Frit 3110 37.04
Ferro Frit 3124 18.52
EPK Kaolin 5.19
Silica (325 mesh) 7.40
Add Amount
Bentonite 1.48
Copper Carbonate 5.93
Red Iron Oxide 2.22

Instructions

This recipe is not food safe. This recipe is nice in Raku. Nice over shiny glazes. Crawly, beaded surface. Shown in the image here on top of a blue terra sigillata and Faux Lead Hulk Smash  glaze and Faux Lead Amber.

Published in "Low-Fire Surfaces" by Ronan Kyle Peterson, in the September 2017 issue of Ceramics Monthly.
Works best layered over Faux Lead glaze. It's dry, flaky, and sharp when used by itself.