All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Cryolite 10.00
Gerstley Borate 20.00
Lithium Carbonate 30.00
Spodumene 15.00
Zircopax 25.00

Instructions

Published in "Low-Fire Sculpture Glazes" by Holly Goring, in the December 2016 issue of Ceramics Monthly.

J.P.'s Dry is a low-fire base glaze for sculpture that holds colorants well. For Patina Green, add: 0.25% Copper Carbonate. For Soft Yellow, add: 6.0% Red Iron Oxide. For Black, add: 6.0% Manganese Carbonate and 7.0% Nickel Oxide. The glaze variation on the test tile shown here is Patina Green.
This glaze is not food safe.