All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
High-Alkaline Frit 75.00
China Clay 15.00
Silica 10.00
Add Amount
Red Iron Oxide 10.00

Instructions

This recipe is from the November/December 2018 issue of Pottery Making Illustrated in the feature, "Developing Color: Yellow Glazes." This article is excerpted from Colour in Glazes by Linda Bloomfield.
Note: Many metal oxides are toxic. Wear protective gloves and a respirator when mixing glazes or stains/washes and make sure your kiln is well ventilated to avoid inhaling fumes from the firing.