All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 9.00
Talc 4.00
Whiting 9.00
High-Alkaline Frit 9.00
Nepheline Syenite 36.00
China Clay 5.00
Silica 28.00
Add Amount
Copper Carbonate 0.50
Tin Oxide 4.00

Instructions

Published in "Red and Orange Glazes" by Linda Bloomfield, in the Sep/Oct 2012 issue of Pottery Making Illustrated.
Use Ferro Frit 3110 when high alkaline frit is listed in a recipe. Note that the frit sometimes causes glazes to craze. To correct this, try substituting a higher boron frit.