All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 12.00
NC-4 Feldspar 28.00
Grolleg Kaolin 50.00
Silica 10.00
Add Amount
Water 40.00

Instructions


This is a modified recipe from Val Cushing’s Handbook. I mix many clay-body recipes into casting slips, even if the original recipe is not designated as a casting body. To create a casting slip from this recipe, add a deflocculant such as Darvan 7 or sodium silicate.

This recipe was shared by David Scott Smith in the November/December 2020 issue of Pottery Making Illustrated.