All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3110 1.00
Custer Feldspar 9.00
Nepheline Syenite 35.00
EPK Kaolin 23.00
OM 4 Ball Clay 25.00
Silica 7.00
Add Amount
Water 42.50
Sodium Silicate 0.25

Instructions


Use 0.25–0.5% sodium silicate.

Recipe from ceramic artist Shalene Valenzuela. Her slip is a modified Hensley/Polseno recipe.

This recipe was shared by David Scott Smith in the November/December 2020 issue of Pottery Making Illustrated.