All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 13.60
Strontium Carbonate 13.60
Whiting 27.30
Ferro Frit 3134 9.10
Ball Clay 27.30
Silica 9.10
Add Amount
Bentonite 2.00
Red Iron Oxide 10.00
Titanium Dioxide 5.00

Instructions

The piece in the image shown here was glazed with Ashleigh's Rivulet and Frasca Ash (green) over Green Dragon Matte glaze.

Originally published in the Sept/Oct 2017 issue of Pottery Making Illustrated.
Warning: Ash glazes and the glaze combinations listed and shown above can and do run during the firing. Plan accordingly to protect your kiln and kiln shelves. Ian Hall-Hough side fires all of his pieces with runny glazes on seashells and wadding, which are then placed and fired on a drip tray (a waster slab that has been bisque fired and is used during the glaze firing to catch the glaze that runs off the pots). After the firing, Ian uses a rubbing stone and/or a Dremel to clean up any sharp edges shells to remove and leftover white powder (calcium oxide) that is left after the firing.