All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 66.00
F-4 Feldspar (Minspar 200) 17.00
Nepheline Syenite 6.00
EPK Kaolin 11.00
Add Amount
Zircopax 10.00
Tin Oxide 5.00
Bentonite 2.00

Instructions

Published in "Full Circle: Majolica Decorating Techniques" by Janice Strawder, in the Nov/Dec 2012 issue of Pottery Making Illustrated.