All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 18.40
Whiting 7.70
Ferro Frit 3134 22.30
Spodumene 28.50
EPK Kaolin 12.00
Silica 11.10
Add Amount
Zircopax 10.00
Bentonite 2.00

Instructions

The local clay here must have a really low thermal expansion because most glazes craze pretty badly. So, I was forced to come up with a really low-expansion, white liner glaze to fit my clay. I usually dip this glaze or use it as a base to layer other glazes on top. 

 

This recipe was shared by Matias Braun in the June/July/August 2024 issue of Ceramics Monthly.