All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 16.30
Whiting 11.96
ferro frit 3124 5.43
Custer Feldspar 44.57
EPK Kaolin 8.70
silica 13.04
Add Amount
BENTONITE 2.17
zircopax 8.70

Instructions

This glaze has a satin finish at cone 5 and a glossy finish when fired to cone 6.

This recipe was shared by Evelyn Ward in the April 2023 issue of Ceramics Monthly.