All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstely Borate 11.00
Strontium Carbonate 6.00
Whiting 8.00
Minspar 200 44.00
Ball Clay 13.00
Silica 18.00
Add Amount
Copper Carbonate 3.00
Iron Oxide 1.00

Instructions

This is a transparent deep glossy green glaze that is low in copper, has a 0.3 RO / 0.7 R2O flux ratio, doesn’t run, has minimal crazing on most clay bodies, and is always magical. Light green when thin and dark when thick. A studio favorite at Ceramics School. Glaze developed by Henry Crissman.

 

This recipe was shared by Henry Crissman in the April 2024 issue of Ceramics Monthly.