All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
soda ash 5.33
Nepheline Syenite 26.67
Kona F-4 Feldspar* 14.67
spodumene 20.00
avery kaolin 13.33
om4 ball clay 20.00

Instructions

*Substitute Minspar 200 feldspar for the Kona F-4 feldspar, which is no longer mined. 

 

This recipe was shared by Dan Anderson in the March 2022 issue of Ceramics Monthly.