All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 4.12
Whiting 14.43
Potash Feldspar 45.37
EPK Kaolin 6.19
Silica 24.74
Zinc Oxide 5.15
Add Amount
mason-stain-6479 12.37
Bentonite 2.06

Instructions

Works well as a relatively glossy base glaze, is very stable, and does not move. Can look good on top of other glazes, but sometimes the yellow gets eaten up by stronger colors. 

For the three or more glaze combination tests, I dipped the entire piece in the first glaze for two seconds, let it dry, then inverted the piece and dipped a second glaze for one second. The pieces were then allowed to dry, at which point a third glaze was applied by inverting the pieces and glazing the top one-quarter for one second. The image shown with this recipe shows Sunshine + Spearmint + Pike's Purple.

This recipe was shared in the January 2025 issue of Ceramics Monthly as an excerpt from Odyssey ClayWorks Director Gabriel Kline’s Amazing Glaze Recipes and Combinations, published by Quarto Press.