All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Potash Feldspar 33.00
Talc 21.00
Flint 16.00
Grolleg 15.00
Whiting 12.00
Zinc Oxide 3.00
Add Amount
Titanium Dioxide 5.00
Red Iron Oxide 4.00

Instructions

speckled brown
stir well