All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
strontium carbonate 25.00
Whiting 7.00
ZInc Oxide 10.00
G-200 Feldspar 45.00
om4 ball clay 13.00
Add Amount
Copper Carbonate 5.00
Red Iron Oxide 1.50
Rutile 1.00

Instructions

Mixing: I usually add the water to a 5-gallon plastic bucket, which can hold a 10,000-gram batch. The water is usually lukewarm to warm, and I always add hard-to-dissolve ingredients like soda ash first. I blunge each ingredient into the glaze with an electric drill and blunger. Once all the ingredients are in the bucket, I continue blunging for 5 minutes. I add just enough water so that when I dip my hand in the glaze, I can see through the glaze to my fingernails. If I cannot see my nails, I keep adding water. If the glaze gets too thin, I let the glaze sit overnight and siphon off water the next day. I then sieve the glaze into a clean 5-gallon bucket.

Application: Apply via dipping or pouring. I prefer letting bisque pieces with wet glazes or slips to dry over- night before applying additional slips or glazes.

Note: Glazes with barium carbonate or high percentages of metallic oxides are generally not food safe.

 

This recipe was shared in the April 2022 issue of Ceramics Monthly.