All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 12.65
ferro frit 3124 32.33
minspar 200 feldspar 25.91
EPK Kaolin 9.63
silica 19.48

Instructions

Add dissolved Epsom salts to flocculate the glaze, which keeps the particles in suspension and prevents settling. This recipe was developed by Michael Sherrill. 

 

This recipe was shared by Charlotte Grenier in the April 2023 issue of Ceramics Monthly.