All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
whiting 20.00
kona f-4 feldspar 30.00
om 4 ball clay 20.00
silica 30.00
Add Amount
bentonite 2.00

Instructions

*Substitute Minspar 200 feldspar for Kona F-4 feldspar. Mix this glaze to a thin consistency. Apply a medium coating via brushing. 

These recipes are shown applied over a dark clay body. I work mainly with a clay body from STARworks called DarkSTAR 10, and I also use other high-fire clays from various clay companies. 

This recipe was shared by Minsoo Yuh in the January 2022 issue of Ceramics Monthly.