All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Soda Ash 3.20
F-4 Feldspar 8.64
Nepheline Syenite 36.00
Spodumene 12.16
EPK Kaolin 28.00
OM 4 Ball Clay 12.00

Instructions

F-4 feldspar is no longer available, so use Minspar 200. This recipe was graciously shared with me by Ryan MacDonnell, ceramics professor at Montgomery College. It produces flashing effects in wood, salt, and soda firings. I have also found that it yields a salt-like effect when used under my Basic Wood Ash Wash. Apply to leather-hard clay.

This recipe was shared by Ian Hall-Hough in the September 2023 issue of Ceramics Monthly.