All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 13.63
Gerstley borate 10.69
Talc (Desert or C-30) 13.10
Custer Feldspar 38.13
OM 4 Ball Clay 6.68
silica 17.77
Add Amount
cobalt carbonate 0.50
Green Chrome 0.50

Instructions

This glaze is fired to cone 10 in reduction in a gas kiln. Works well layered over Zacks Black. 

 

This recipe was shared by Mark Cortright in the October 2021 issue of Ceramics Monthly.