All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 13.00
Lithium Carbonate 2.00
strontium carbonate 4.00
Whiting 11.00
Custer Feldspar 49.00
silica 21.00
Add Amount
BENTONITE 2.00
Copper Carbonate 5.00
Titanium Dioxide 4.00
Shark Fin Recipe

Instructions

This is a stable, workhorse of a glaze that can be dipped, brushed, or poured. Mix it to the consistency of whole milk. 

 

This recipe was shared by Mariana Baquero in the Nov/Dec 2022 issue of Pottery Making Illustrated.