All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 26.21
ferro frit 3124 34.95
EPK Kaolin 33.99
silica 4.85
Add Amount
Black Copper Oxide 2.43

Instructions

This recipe was developed by Tony Hansen (DigitalFire.com). 

 

This recipe was shared by Charlotte Grenier in the April 2023 issue of Ceramics Monthly.