All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 30.00
Ferro Frit 3195 50.00
EPK Kaolin 20.00

Instructions

I brush, pour, and dip this glaze, keeping it somewhat thick. It stays matte and dry just under cone 04 but can run if it’s very thick and gets too hot.

 

This recipe was shared by Maggie Jaszczak in the March 2024 issue of Ceramics Monthly.