All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Strontium Carbonate 12.33
Wollastonite 18.49
Ferro Frit 3195 6.96
Soda feldspar 21.67
EPK Kaolin 15.40
silica 25.15
Add Amount
Chrome Oxide 0.25

Instructions

This glaze should be mixed slightly thinner (toward skim-milk consistency). It can be a runny glaze, especially when applied thick. For the soda feldspar, try Minspar 200 feldspar. 

 

This recipe was shared by Matthew Eames in the October 2022 issue of Ceramics Monthly.